Characteristics of the material VSt6sp   ( VSt6sp,   ВСт6сп ).

Material : VSt6sp   ( VSt6sp,   ВСт6сп )
Substitute: ВСт5сп
Classification : Normal quality structural carbon steel


Chemical composition in % of the material VSt6sp   ( VSt6sp,   ВСт6сп ) .
C Si Mn Ni S P Cr Cu As
0.38 - 0.490.15 - 0.350.5 - 0.8max   0.3max   0.05max   0.04max   0.3max   0.3max   0.08


Temperature of critical points of the grade VSt6sp   ( VSt6sp,   ВСт6сп ).
Ac1 = 725 ,      Ac3(Acm) = 790 ,       Ar3(Arcm) = 780 ,       Ar1 = 690


Mechanical properties under Т=20oС of the material VSt6sp   ( VSt6sp,   ВСт6сп ) .
Assortment Dimension Direct. sв sT d5 y KCU Heat treatment
- mm - MPa MPa % % kJ / m2 -
Rolled stock     535 325 25 52630 


Physical properties of the material VSt6sp   ( VSt6sp,   ВСт6сп ) .
T E 10- 5 a 10 6 l r C R 10 9
Grade MPa 1/Grade Watt/(m·Grade) kg/m3 J/(kg·Grade) Ohm·m
20 1.97          
100 1.97          
200 1.86          
300 1.75          
400 1.68          
T E 10- 5 a 10 6 l r C R 10 9


Technological properties of the material VSt6sp   ( VSt6sp,   ВСт6сп ) .
  Weldability: limited weldability.
 Flakes : not predisposed
Temper brittleness: not predisposed



Specification :
Mechanical properties :
sв - Tensile strength , [MPa]
sT - Yield stress, [MPa]
d5 - Specific elongation at fracture , [ % ]
y - Reduction of area , [ % ]
KCU - Impact strength , [ kJ / m2]
HB - Brinell hardness , [MPa]

Physical properties :
T - Test temperature , [Grade]
E - Young modulus , [MPa]
a - Coefficient of linear expansion (range 20o - T ) , [1/Grade]
l - Termal (heat) condition coefficient , [Watt/(m·Grade)]
r - Density , [kg/m3]
C - Specific heat ( range 20o - T ), [J/(kg·Grade)]
R - Electrical resistance , [Ohm·m]

Weldability :
without limitations - welding is done without heating and subsequent heat treeting
limited weldability - welding is possible under heating up to 100-120 grade and subsequent heat treeting
hard weldability - obtaining the quality welding needs the additional operations:heating up to 200-300 grade; the heat treeting ia annealing

Database of steels and alloys (Marochnik) contains information about chemical composition and properties of 1500 steels and alloys (stainless steel, alloy steel, carbone steel, structural steel, tool steel, cast iron, aluminum alloy, titanium alloy, copper alloy, nickel alloy, magnesium alloy and others).
Helpfull for specialists in material technology, structural engineer, mechanical engineer, metallurgy and metal trader

Top

©   2003 - 2009   All rights reserved.       About program.
The entire risk as to use of the Database of Steel and Alloy (Marochnik) content is assumed by you the user

Информация взята с сайта Марочник стали и сплавов


Главная | Новости | Марочник сталей | Контакты | Обратная связь
© 2002 - 2009 Мосспецсталь. Все права защищены
 
-12345-